July 26, 2025
Slurry formulations | ||||||
Sample 4007 | sample 707 | Anjeka 6150 | Anjeka 6043A | Blank | Remark | |
Resin | 36 | 36 | 36 | 36 | 36 | PVC Paste Resin |
Plasticisers
|
23.5 | 23.5 | 23.5 | 23.5 | 23.5 | DOP |
Dispersant | 0.5 | 0.5 | 0.5 | 0.5 | ||
Titanium dioxide | 40 | 40 | 40 | 40 | 40 | 龙蟒R996 |
Total | 100 | 100 | 100 | 100 | 100 |
Add the dispersant to the resin and mix well, add titanium dioxide and then use a dispersion machine 2500RAM to disperse for 5 minutes.
Comparison of viscosity reduction of different dispersants | ||
30℃,mpa.s | Initial Viscosity | Viscosity after 24H |
Blank | 38000 | 45000 |
Sample 4007 | 32000 | 34200 |
Sample 707 | 31000 | 33520 |
6150 | 5200 | 6200 |
6043A | 6000 | 7360 |
In PVC paste resin white slurry, the viscosity reduction effect of Anjeka Dispersant 6150 6043A was better than that of the sample.
Slurry formulation | ||||||
Sample 4007 | Sample 707 | Anjeka 6150 | Anjeka 6043A | blank | Remark | |
Resin | 36 | 36 | 36 | 36 | 36 | PVC Paste Resin |
Plasticiser | 23.6 | 23.6 | 23.6 | 23.6 | 23.6 | DOP |
Dispersant | 0.4 | 0.4 | 0.4 | 0.4 | ||
calcium | 40 | 40 | 40 | 40 | 40 | 1250 mesh |
Total | 100 | 100 | 100 | 100 | 100 |
Add the dispersant to the resin and mix well, add the heavy calcium and then use the disperser to disperse for 5 minutes at 2500RAM.
Comparison of viscosity reduction of different dispersants | |
30℃,mpa.s | viscosity |
Blank | 8000 |
Sample 4007 | 4637 |
Sample 707 | 4732 |
6150 | 4951 |
6043A | 4808 |
In PVC paste resin filler slurry, Angelcon dispersant 6150 6043A viscosity reduction effect to sample is very close.