Latest company cases about Defoamer Test	 For Two-Component Black Polyurethane Topcoat
Two-Component Black Polyurethane Topcoat Defoamer Test
May 26,2026
Test Procedures
  1. Two-component black polyurethane topcoat test in 100ml graduated cylinder: original graduation, foam suppression height after shaking evenly, graduation after defoaming Time after defoaming, surface tension.
  2. Add 50g two-component black topcoat into the cylinder respectively, add TEGO810, TEGO902, BYK028, BYK024 Anjeka 5062A, Anjeka 5063, Anjeka 26022801 (New) comparative test. Defoamer dosage: 0.1%-0.2%
  3. Squeegee comparative cratering test, Paint: Curing Agent = 4:1
Paint Formulation
Component Value Unit/Note
Two-Component Black Polyurethane Topcoat

Water 3
3639H Waterborne Acrylic Dispersion 70 (Double Bond)
DPNB Solvent Dipropylene Glycol Butyl Ether 5
DB Solvent Diethylene Glycol Butyl Ether 3
DPM Solvent Dipropylene Glycol Methyl Ether 3
190 Dispersant MA-100/15% Black Paste 16
Total 100
Defoamer Test Results
0.1% Defoamer Dosage (50g black paint with 0.05g defoamer)
Defoamer Name Added to Black Paint Manufacturer Original Graduation Foam Suppression Heigh Height After Defoaming Approximate Time Surface Tension Foam Generation Volume
Two-Component Black Paint Without Defoamer
49.5 50 49.5 1.5h 23.23 0.5
TEGO810 TEGO 49.5 50 49 1.5h 19.73 1
TEGO902 TEGO 49.5 50 49 1.5h 16.68 1
BYK028 BYK 49.5 50 49.5 1.5h 19.13 0.5
BYK024 BYK 49.5 51 49 1.5h 17.33 1
5062A Anjeka 49.5 50 49 1.5h 11.93 1
5063 Anjeka 49.5 53 49 1.5h 11.75 4
5061 Anjeka 49.5 50 49.5 1.5h 15.92 0.5
5064 Anjeka 49.5 51 50 1.5h 14.17 1

In terms of foam suppression, 5063 shows the worst performance, 5061 the best, with others being consistent; defoaming time of all samples is consistent with the base paint; in terms of surface tension, 5062A and 5063 show the lowest values.

0.2% Defoamer Dosage (50g black paint with 0.1g defoamer)
Defoamer Name Added to Black Paint Manufacturer Original Graduation Foam Suppression Heigh Height After Defoaming Approximate Time Surface Tension Foam Generation Volume
Two-Component Black Paint Without Defoamer
49.5 51 49 1.5h 22.47 1
TEGO810 TEGO 49.5 49.5 49 1.5h 16.77 0.5
TEGO902 TEGO 49.5 49.5 49 1.5h 15.75 0.5
BYK028 BYK 49.5 50 49 1.5h 19.74 1
BYK024 BYK 49.5 49.5 49 1.5h 14.49 0.5
5062A Anjeka 49.5 50 49 1.5h 13.09 1
5063 Anjeka 49.5 50 49 1.5h 16.93 1
5061 Anjeka 49.5 50 49 1.5h 16.73 1
5064 Anjeka 49.5 50 50 1.5h 15.01 0

In terms of foam suppression, 5064 shows the best performance; in terms of defoaming power, 5062A is the strongest; defoaming time of all samples is consistent with the base paint; in terms of surface tension, 5062A shows the lowest value.

Cratering Test Results
Defoamer Name Added to Black Paint Manufacturer 0.1% Dosage 0.2% Dosage
thickness um gloss Cratering (Yes/No) thickness um gloss Cratering (Yes/No)
Two-Component Black Paint Without Defoamer
14.5 81.3/52.3 No 14.5 81.2/55.5 No
TEGO810 TEGO 27 76.9/37.6 Yes 21 84.8/65.8 Yes
TEGO902 TEGO 24 88.6/54.7 No 22 83.6/63.6 Yes
BYK028 BYK 23 81/52.7 No 18 66.5/32.5 No
BYK024 BYK 18 82/55.4 No 17 76.3/34.7 Yes
5062A Anjeka 21 84.6/46.5 Yes 16 82.1/60.2 Yes
5063 Anjeka 24 84.1/57.6 Yes 17 86.8/73.1 Yes
5061 Anjeka 21 87/71.3 Yes 22 84.4/63.2 Yes
5064 Anjeka
88.3/64.9 Yes
88.165.4 Yes

Based on the comprehensive test results, 5062A offers the strongest defoaming power, suitable for systems requiring fast defoaming; 5064 delivers the best gloss and excellent foam suppression, suitable for topcoat systems with high surface appearance requirements. Both are recommended.

Cratering Test with Wetting Agent
0.2% Defoamer Dosage, 0.3% Wetting Agent Dosage
Defoamer Name Added to Black Paint Manufacturer Wetting Agent Details
thickness um Wetting agent Model 60°/20°gloss Cratering (Yes/No)
Two-Component Black Paint Without Defoamer


81.3/52.3 No
TEGO810 TEGO 27 4100 78.5/42.8 Yes
TEGO902 TEGO 24 4100 88.6/54.7 No
BYK028 BYK 23 349 81/52.7 No
BYK024 BYK 18 349 82/55.4 No
5062A Anjeka 21 7425A 84.1/57 Yes
5063 Anjeka 24 7425A 84.2/42.2 Yes
5061 Anjeka 21 7425A 87/71.3 Yes
5064 Anjeka
7422 88.3/65.6 No
5063 Anjeka
7334 88.2/70.8 No
5062A Anjeka
7334 90/77.1 No

After wetting agent addition, 5064 shows the highest gloss. For 5063 and 5062A, adding 7334 can effectively resolve the cratering issue when it occurs.

0.2% Defoamer Dosage, 0.3% Wetting Agent Dosage (Continued)
Defoamer Name Added to Black Paint Manufacturer Wetting Agent Details
thickness um Wetting agent Model 60°/20°gloss Cratering (Yes/No)
Two-Component Black Paint Without Defoamer




TEGO810 TEGO 12 4100 87.1/74.1 Yes
TEGO902 TEGO 14 4100 84.9/70.9 No
BYK028 BYK 17 349 85.2/54.6 No
BYK024 BYK 18 349 86/48.8 No
5062A Anjeka 12.4 7422 87.1/66.6 No
5063 Anjeka 15 7422 81.9/58.9 No
5061 Anjeka 16.3 7422 89.2/75.1 No
5064 Anjeka
7422 87.5/64.5 No
5063 Anjeka
7334 88.5/69.5 No
5062A Anjeka
7334 90.8/70.1 No

Summary: 5064 generally shows higher gloss but weaker defoaming performance. For 5062A and 5063, when cratering cannot be resolved, adding 7334 can effectively improve the issue.